Global Global Algérie Français Algeria English Angola Português Angola English Argentina Español Argentina English Australia English Austria Deutsch Austria English Azerbaijan English Azerbaijan Русский Bahrain English Bangladesh English Belgium English Belgium Français Belgium Nederlands Brazil Português Brazil English Bulgaria български Bulgaria English Cameroon English Cameroon Français Canada English Canada Français Chile Español Chile English China 中文 China 日本語 China English Colombia Español Colombia English Croatia English Czech Republic Čeština Czech Republic English Denmark English Djibouti English Ecuador Español Ecuador English Egypt English Estonia English Ethiopia English Finland Suomi Finland English France Français France English Georgia English Georgia Русский Germany Deutsch Germany English Ghana English Greece Ελληνικά Greece English Guatemala Español Guatemala English Hong Kong, China English Hong Kong, China 中文 Hungary Magyar Hungary English India English Indonesia English Iraq English Ireland English Italy Italiano Italy English Ivory Coast Français Ivory Coast English Japan 日本語 Japan English Jordan English Kazakhstan Русский Kazakhstan English Kenya English Kuwait English Kyrgyzstan Русский Kyrgyzstan English Latvia English Lithuania English Malaysia English Mauritius English Mauritius français (Maurice) Mexico Español Mexico English Moldova Română Moldova English Mongolia English Morocco English Morocco Français Mozambique Português Mozambique English Netherlands Nederlands Netherlands English New Zealand English Nigeria English Norway English Oman English Pakistan English Paraguay Español Paraguay English Peru Español Peru English Philippines English Poland Polski Poland English Portugal Português Portugal English Qatar English Republic of Korea 한국어 Republic of Korea English Romania Română Romania English Saudi Arabia English Serbia Српски Serbia English Singapore English Slovakia English Slovenia English South Africa English Spain English Spain Español Sri Lanka English Sweden English Switzerland Deutsch Switzerland Français Switzerland Italiano Switzerland English Tanzania English Thailand ไทย Thailand English Togo English Togo Français Tunisia English Tunisia Français Türkiye Türkçe Türkiye English Turkmenistan Русский Turkmenistan English Ukraine Українська Ukraine English United Arab Emirates English United Kingdom English Uruguay Español Uruguay English USA English Uzbekistan English Uzbekistan Русский Vietnam Tiếng Việt Vietnam English

Machine-direction breaking length is one of the most important strength indices for corrugating medium (corrugated base paper), directly reflecting the tensile integrity that supports flute formation and box compression performance. This article explains the definition, calculation principle, sample preparation, reference standards such as ISO 1924-2 and GB/T 12914, testing procedures, and typical applications of MD breaking length determination for corrugated base paper. It is intended for quality engineers, laboratory technicians, and sourcing specialists in the pulp, paper, and packaging industries.

Technical Overview

Breaking length is a normalized tensile parameter that expresses the tensile strength of paper relative to its own weight. It is defined as the theoretical minimum length of a uniform paper strip, suspended vertically from one end, at which the strip would break under its own mass. Because the calculation divides the measured breaking force by both specimen width and grammage, breaking length is independent of sample dimensions and allows meaningful comparison between papers of different basis weights.

For corrugating medium, the machine direction (MD) is of particular interest. During papermaking, the majority of fibers orient along the machine direction, so MD tensile strength is significantly higher than cross-direction (CD) strength. When the medium is fluted and converted into corrugated board, the machine direction of the sheet corresponds to the height direction of the finished box, meaning MD tensile integrity contributes directly to edgewise compression resistance and stacking strength. For this reason, the Chinese national product standard for corrugated base paper, GB/T 13023, designates MD breaking length as a key quality index for grade classification and acceptance.

The parameter is calculated from the tensile breaking force as follows: L = 1000 × F / (9.81 × G × b), where L is the breaking length in kilometers, F is the average breaking force in newtons, G is the grammage in grams per square meter, and b is the specimen width in millimeters. Breaking length can also be derived from the tensile index I (in N·m/g) using the relation L (km) = I / 9.81.

Testing Samples

Product Forms and Grades

Typical test articles include corrugating medium in roll or sheet form, with grammages commonly ranging from approximately 80 g/m² to 200 g/m². Both recycled-furnish and virgin semichemical grades are covered, and all commercial quality levels may be evaluated. Samples should be taken from positions representative of the full production width, avoiding damaged edges, splices, and visibly defective areas.

Specimen Preparation

  • Cut at least 10 test strips with their long axes precisely parallel to the machine direction.
  • Preferred dimensions per ISO 1924-2: width 15.0 mm ± 0.1 mm and length of at least 250 mm to accommodate a 180 mm test span.
  • Strips must be free from wrinkles, creases, watermarks, and pinholes, with clean, parallel, burr-free edges produced by a sharp knife or precision sample cutter.
  • Mark the machine direction on each specimen and avoid touching, bending, or contaminating the test region during handling.

Conditioning

All specimens must be conditioned to moisture equilibrium in the standard atmosphere specified in ISO 187 or its Chinese equivalent GB/T 10739, namely 23 °C ± 1 °C and 50 % ± 2 % relative humidity. Conditioning is typically maintained for at least several hours, with longer times for heavier grammages, and all testing should be performed in the same controlled atmosphere to ensure reproducibility.

Testing Items

Primary Parameter

The principal deliverable is the machine-direction breaking length of the corrugating medium, expressed in kilometers or meters, reported as the mean of all valid specimen breaks.

Associated Measured and Calculated Outputs

  • Individual and average breaking force (N) of MD specimens.
  • MD tensile strength (kN/m), calculated as breaking force divided by specimen width.
  • MD tensile index (N·m/g), tensile strength divided by grammage.
  • Elongation at break (%) where the tensile tester supports extension measurement.
  • Grammage (g/m²) determined separately per ISO 536 or GB/T 451.2, as it is an essential input to the breaking length calculation.
  • Statistical summary including standard deviation, coefficient of variation, minimum and maximum values, and the number of valid breaks.

Testing Methods

Reference Standards

The determination is most commonly performed in accordance with ISO 1924-2 (Paper and board — Determination of tensile properties — Constant rate of elongation method at 20 mm/min) or GB/T 12914, the Chinese standard for tensile properties of paper and board that is widely applied in domestic trade. ISO 1924-3, which specifies a higher constant rate of elongation, and TAPPI T 494 are also recognized internationally. The method actually used must always be stated in the test report, since specified test speeds and specimen widths may differ between standards.

Apparatus

Testing requires a constant-rate-of-elongation (CRE) tensile testing machine with calibrated force measurement, adjustable clamps, and an initial test span of 180 mm ± 2 mm. The crosshead speed is set to 20 mm/min per ISO 1924-2. A precision specimen cutter or a metal template with a sharp cutting blade is used for strip preparation, and a calibrated balance is required for grammage verification.

Test Procedure

  • Verify the calibration status of the tensile tester and set the gauge length to 180 mm.
  • Insert one end of the conditioned MD strip into the upper clamp, align it vertically without twisting, and secure it with consistent clamping pressure.
  • Clamp the lower end, applying just sufficient tension to remove slack, and start the test at 20 mm/min.
  • Record the maximum force at rupture; specimens that slip in the clamps or break within approximately 10 mm of a jaw line are rejected and replaced until at least 10 valid results are obtained.
  • Calculate tensile strength, tensile index, and breaking length for each valid specimen, then average the results.

Calculation and Reporting

The test report should identify the sample and its source, the conditioning atmosphere and duration, the testing standard applied, the verified grammage, specimen width and span, the number of valid breaks, the individual and mean breaking forces, the calculated MD breaking length (normally to two decimal places in kilometers), and the statistical dispersion. Any deviations from the standard method must be documented.

Applications

  • Incoming inspection of corrugating medium by corrugators and sheet plants to verify strength claims before fluting on the corrugator.
  • Grade classification and conformity assessment against GB/T 13023 and against purchase specifications in domestic and international trade.
  • Mill process optimization, including refining energy, furnish composition, recycled fiber ratio, wet pressing, sizing, and strength additive dosage.
  • Research and development of new medium grades, and correlation studies linking MD breaking length with short-span compression, cone crush, and finished box compression performance.
  • Failure analysis when corrugated boxes underperform in burst, edgewise crush, or stacking tests.
  • Independent verification, batch certification, and dispute resolution through accredited third-party laboratories issuing standards-based test reports.

FAQ

Why is the machine direction specified rather than the cross direction?

Because fibers align predominantly along the machine direction, and in a converted corrugated box the MD of the medium runs in the column height direction, MD tensile strength governs the contribution of the medium to compression and stacking performance. GB/T 13023 therefore controls MD breaking length as the primary index.

What breaking length values are typically required?

Requirements depend on product grade and grammage; commercial specifications for corrugating medium commonly call for MD breaking lengths in the approximate range of 2.0 km to 4.5 km. The applicable minimum should always be confirmed against the grade tables of GB/T 13023 and the specific purchase contract.

How does moisture affect the result?

Tensile strength of paper falls noticeably as equilibrium moisture content rises, so unconditioned or inconsistently conditioned samples can produce misleadingly low or scattered results. Strict adherence to the 23 °C and 50 % RH standard atmosphere is essential for comparability between laboratories.

How is breaking length related to tensile index?

The two parameters are directly interchangeable: breaking length in kilometers equals the tensile index in N·m/g divided by 9.81. Reporting both makes results easier to compare across grammages and between suppliers.

Which test methods are mutually recognized?

ISO 1924-2, GB/T 12914, and TAPPI T 494 are all based on the CRE principle and yield comparable data, but because test speed and specimen dimensions differ, the method used must be declared and kept consistent when comparing datasets or historical trends.